1.2344 Hot Work Mold Steel
One. Product Description
1.2344 is German brand, which is a Pressure-Resistant Hot Work Mold Steel. The steel after electroslag remelting is uniform in material, good in hardenability, excellent in machining performance and polishing performance, high in toughness and plasticity, good in high and low temperature wear resistance, high temperature fatigue resistance and heat resistance.
Two. Quality Standard
EN ISO 4957 Standard Specification for Tool Steels
Three. Product Specifications
Four. Equivalent Grade of 1.2344 Mold Steel - For Reference Only
|
China GB |
Germany DIN |
US AISI |
Japan JIS |
EU EN |
1.2344 |
4Cr5MoVSi |
1.2344 |
H13 |
SKD61 |
X37CrMoV5-1 |
Five. Product Features and Uses
Features:
1. High heat resistance hot work mold steel.
2. Excellent toughness and ductility in all directions.
3. High thermal fatigue resistance and wear resistance.
4. Nitriding can be applied.
5. Good polishability.
6. Good dimensional stability.
7. Better hardenability.
8. Better isotropy than conventional melting steel.
9. Can also be used for cold working.
Use:
1. Suitable for Mold-casting mold, hot forging mold, hot extrusion mold.
2. For high wear-resistant plastic molds, such as automobile tire alloy rings, engines, fishing reels.
Six. Product Detailed Information
1.2344 is a German brand, which is a pressure-resistant hot work mold steel. The steel after electroslag remelting is uniform in material, good in hardenability, excellent in machining performance and polishing performance, high in toughness and plasticity, good in high and low temperature wear resistance, and good in high temperature fatigue resistance and heat resistance.
The company adopts pure alloy melting, advanced alloy electroslag remelting, large-scale three-dimensional isotropic forging and unique heat treatment process. The company's sales network covers dozens of countries and regions in Europe, North America, and Asia. In recent years, it has become the exclusive mold-casting mold material supplier for many large-scale Mold-casting mold manufacturers in Germany. World-renowned companies such as Volkswagen, Mercedes-Benz and BMW all directly purchase mold-casting mold materials from CapitaLand.
Heat Treatment:
Ingot casting: heating temperature 1180~1200℃, starting temperature 1130~1150℃, ending temperature ≥850℃, pit cooling.
Steel billet: heating temperature 1120~1160℃, starting temperature 1070~1110℃, ending temperature ≥850℃, sand cooling or slow cooling.
Isothermal Annealing Specifications:
Annealing temperature (850±10)℃, hold for 2h, cool to (720±10)℃ with the furnace, hold for 4h, cool in the furnace to below 500℃, air cooling, hardness ≤229HBW.
High Temperature Tempering Specifications:
Tempering temperature (730±10)℃, holding for 2h, furnace cooling ≤500℃, air cooling.
Quenching and Tempering Specifications:
Quenching temperature 850~880℃, oil cooling, hardness 50~52HRC; tempering temperature 580~640℃, air cooling, hardness 28~36HRC.
Pre-Hardening Treatment Specifications:
Heating temperature 860~900°C, oil cooling, tempering temperature 570~700°C, air cooling, tempering hardness 28~35HRC.